Mixing

  • Follow the ratio exactly. Most 2-part systems are mixed by volume (e.g. 1:1 or 2:1) or by weight. Use the correct parts and a clean, dedicated container.
  • Mix thoroughly but gently. Under-mixing leaves unmixed resin that never cures (soft patches). Over-mixing at high speed whips in air (bubbles).
  • Scrape the sides and bottom of the container — the unmixed material is always there.
  • Kiss-and-mix for small batches: mix, apply a little, mix more, apply more.

Pot life and planning

Pot life is how long the mixed material stays workable. It’s temperature-dependent — warmer = shorter pot life. Plan your area so you can mix, spread and finish a section before the material starts to gel.

  • On a big floor, work in sections you can actually complete.
  • Have your tools (roller, squeegee, spike) ready and the next batch prepped before you start.
  • If you’re running out of pot life, stop — a gelled, trowelled patch is a visible, permanent defect.

The application sequence

  1. Primer / base coat (if the system uses one) — thin, even, full coverage. Let it cure to the spec.
  2. Main coat — apply with a squeegee for even thickness, then cross-roll to remove marks.
  3. Top coat / wear layer (if specified) — adds chemical and abrasion resistance.
  4. Cure — hold traffic to the manufacturer’s schedule. Rushing cure is a classic cause of early failure.

The five common defects — and their causes

DefectUsual causePrevention
BubblesAir trapped in mix or on surfaceMix gently, de-aerate, cross-roll, use a spike
PinholesAir rising through the coating, or contaminationDegrease substrate, apply even film, let degas
Roller marksInconsistent roller pressure, low filmCross-roll, keep a wet edge, sufficient material
Holidays (missed spots)Uneven coverage, running out of materialOverlap sections, keep a wet edge, plan batches
Poor adhesion / delaminationMoisture, poor profile, contaminationTest moisture, verify profile, degrease

Checklist: Mix to spec, work within pot life, apply in sections you can finish, cross-roll, and respect the cure schedule. The defects are almost never mysterious — they’re almost always a step you rushed.

Key takeaways

  • Mix by volume or weight exactly as specified — never 'eyeball' it.
  • Respect pot life: plan your area so you can finish before the material gels.
  • Most defects are preventable: bubbles, pinholes and roller marks all trace back to prep or technique.